Incoloy 800H exists for one reason: creep strength above 600 °C. It is the controlled-carbon, controlled-grain-size variant of Incoloy 800 (UNS N08810 vs N08800), designed so that the material keeps its shape and load capacity during long, hot service, the duty of steam methane reformer tubes, ethylene cracking furnace tubes and power-plant superheaters. The verified anchors are a service ceiling of 1100 °C and a density of 7.94 g/cm³; the creep performance itself rests on two specification levers, carbon content and grain size, both of which must appear on the certificate.
What creep and rupture actually mean here
Creep is time-dependent deformation under load at temperature: a tube held at 900 °C under internal pressure slowly stretches, and the useful question is not the room-temperature tensile strength but the stress it can carry for a design life without exceeding an allowable strain or reaching rupture. Stress-rupture is the time to fracture at a given stress and temperature. Above roughly 600 °C these two properties, not yield strength, size the component, which is why 800H is specified where 800 would be marginal. This site documents 800H to a verified ceiling of 1100 °C, with the enhancement versus 800 stated explicitly above 600 °C.
The two levers: carbon and grain size
800H is the controlled-carbon 800: the carbon range is held higher and narrower than in 800 so that fine carbides stabilise the structure at temperature, and the alloy is supplied solution annealed with a grain size of ASTM 5 or coarser: the coarse grain is the creep-strength feature. This is why the grain-size requirement belongs on the purchase order: a heat that is otherwise “800H chemistry” but fine-grained will not deliver the creep behaviour the grade is chosen for. The related verified design features are controlled carbon for carburization resistance and good structural stability at temperature.
The code basis: ASME Section III and VIII
800H is qualified for ASME Section III and Section VIII pressure-vessel service, which is the framework that publishes the allowable stresses a designer works to. The form standards are ASTM B163 (seamless pipe and tube) and ASTM B407 (nickel-iron-chromium seamless pipe and tube), with the ASME SB-163 / SB-407 twins used in pressure-code work. In practice the specification chain is: grade UNS N08810, form standard B163/B407 (or ASME SB-163/SB-407), condition solution annealed, grain size ASTM 5 or coarser, and certificate EN 10204 3.1 with heat chemistry that proves the carbon and the grain size.
How to specify 800H for a creep duty
State the peak metal temperature and the design life first, they decide whether 800H or a higher-strength grade (625 at 980 °C, or a cobalt grade) is required. Then specify: Incoloy 800H, UNS N08810 (GB NS1102), form standard ASTM B163 / B407 or ASME SB-163 / SB-407, condition solution annealed with grain size ASTM 5 or coarser, and certificate EN 10204 3.1 with the carbon content and grain size reported against the heat. Use the RFQ spec writer to assemble the enquiry, and the service-temperature lookup to compare the ceilings of the stocked grades.
How to select the right option for your process
Run the list top to bottom before the enquiry goes out, that is what keeps the part inside its specification:
- Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
- Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
- Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
- Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
- Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.
Frequently Asked Questions (FAQ)
What is the maximum service temperature of Incoloy 800H?
The verified ceiling on this site is 1100 °C. Above about 600 °C 800H is chosen over Incoloy 800 specifically for its enhanced creep and stress-rupture strength.
Why does grain size matter for 800H?
800H is supplied solution annealed with a grain size of ASTM 5 or coarser; the coarse grain is the creep-strength feature. A fine-grained heat will not deliver the creep behaviour the grade is specified for, so the grain-size requirement belongs on the purchase order and certification.
How is 800H different from 800?
800H (UNS N08810) is the controlled-carbon variant of 800 (N08800) with a specified coarse grain size to enhance creep and stress-rupture strength, and reaches its advantage above roughly 600 °C. Both share the Ni-Fe-Cr base.
Which standards govern 800H tube?
ASTM B163 (seamless nickel-chromium-iron pipe and tube) and ASTM B407 (nickel-iron-chromium seamless pipe and tube), with ASME SB-163 / SB-407 as the pressure-code twins. ASME Section III and VIII provide the design-allowable basis.