Maximum magnetic flux in minimum weight (2.4 T saturation), or maximum permeability for transformer and shield cores?

1J22 (HiperCo 50 equivalent) is an iron-cobalt-vanadium soft magnetic alloy offering the highest saturation magnetic induction (2.4 T) of any commercial magnetic material.

Route the decision

  • If the design must carry the highest flux density in the least mass, solenoid armatures, pole pieces, magnetic bearings, aircraft power generation, take 1J22 (HiperCo 50 equivalent): the highest saturation induction of any commercial soft magnetic material at 2.4 T, with a 940 °C Curie temperature.
  • If the design needs high permeability and low coercivity, instrument transformer cores, magnetic amplifiers, relay armatures, shielding, take 1J50: initial permeability above 30,000 with coercivity below 8 A/m, per GB/T 14986 and IEC 60404-8-6.
  • If high-temperature magnetic performance decides, 1J22’s verified 940 °C Curie temperature is far above 1J50’s operating comfort zone, the aerospace actuator lane.
  • If cold formability into laminations decides, 1J50 lists good cold formability as a verified feature, the lamination and core-stamping lane 1J22 does not target.
Property1J221J50
UNS / GBn/an/a
Density8.2 g/cm³8.2 g/cm³
Max service temp450 °C450 °C
Governing standardsGB/T 14986, AMS 7717 equivalent, ASTM A801GB/T 14986, IEC 60404-8-6
Stock formsWire, Strip, Plate & Sheet, Bar & RodWire, Strip, Plate & Sheet, Bar & Rod

Specification signals

1J22 wins the flux-density axis: 2.4 T saturation induction, the highest of any commercial soft magnetic material, with the 940 °C Curie temperature and aerospace solenoid pedigree under GB/T 14986 and ASTM A801. 1J50 wins the permeability axis: initial permeability above 30,000 and coercivity below 8 A/m, with good cold formability for laminations, the transformer-core and shielding standard under GB/T 14986 and IEC 60404-8-6.

  • 1J22: 1J22 wins the flux-density axis: 2.4 T saturation induction, the highest of any commercial soft magnetic material, with the 940 °C Curie temperature and aerospace solenoid pedigree under GB/T 14986 and ASTM A801.
  • 1J50: 1J50 wins the permeability axis: initial permeability above 30,000 and coercivity below 8 A/m, with good cold formability for laminations, the transformer-core and shielding standard under GB/T 14986 and IEC 60404-8-6.

Switch triggers

Move 1J50 to 1J22 when the design is weight- or volume-critical and needs maximum flux, aerospace actuators, magnetic bearings, and move 1J22 to 1J50 when the duty is permeability-driven, transformer cores, amplifiers, shields, and formability into laminations matters.

How to select the right option for your process

Run the list top to bottom before the enquiry goes out, that is what keeps the part inside its specification:

  1. Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
  2. Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
  3. Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
  4. Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
  5. Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.

Frequently Asked Questions (FAQ)

1J22 or 1J50 for a solenoid armature?

1J22 for a weight-critical aerospace armature, 2.4 T saturation moves the most flux per gram. For a general-purpose relay armature where cost and formability matter, 1J50 serves.

Which has the higher saturation induction?

1J22, at 2.4 T, verified as the highest saturation induction of any commercial soft magnetic material. 1J50’s strength is permeability (above 30,000), not saturation.

Which is better for magnetic shielding?

1J50, shielding works by permeability, and its verified initial permeability above 30,000 with coercivity below 8 A/m is exactly that mechanism. 1J22’s 2.4 T saturation does not shield by itself.

Both under the same standard?

Both cite GB/T 14986, and 1J50 adds IEC 60404-8-6 and 1J22 adds the ASTM A801 / HiperCo 50 equivalent route. Same standard family, different property classes.