Hastelloy C-22 and Hastelloy C-276 sit in the same Ni-Cr-Mo family and look identical on a finished part, yet they are different grades with different jobs: C-276 (UNS N10276) carries the higher molybdenum and is the reference for strongly reducing hot acids, while C-22 (UNS N06022) trades molybdenum for chromium and wins in oxidising and mixed-acid service. The decision is not “which is better” but “which oxidation state does my liquor run at”. This page states the composition windows, the media routing, the pitting index that appears to contradict the field answer, and the one verification step that keeps the two apart at goods-in.
C-22 vs C-276, the composition that decides it
Both windows are published in ASTM B575 (plate, sheet, strip), the standard the two grades share:
| Element (wt %) | C-22 · UNS N06022 | C-276 · UNS N10276 |
|---|---|---|
| Ni | Balance | Balance |
| Cr | 20.0-22.5 | 14.5-16.5 |
| Mo | 12.5-14.5 | 15.0-17.0 |
| W | 2.5-3.5 | 3.0-4.5 |
| Fe | 2.0-6.0 | 4.0-7.0 |
| C | ≤ 0.015 | ≤ 0.010 |
Read the table as a single trade: chromium against molybdenum. Chromium builds the passive film that resists oxidising attack, molybdenum (with tungsten) carries the resistance to reducing acids and to localised attack. C-22 is the chromium-rich side of that trade, C-276 the molybdenum-rich side. Note that both grades contain tungsten: it is not a marker for either one, which is exactly why the two cannot be told apart by a spot test.
Which media routes to which grade
The site’s verified record for C-22 lists FGD scrubbers, pharmaceutical equipment, chemical reactor vessels, pulp and paper bleach plants and waste treatment as its applications, all of them oxidising or mixed-acid duties. Route your duty against that pattern:
| Environment | C-22 | C-276 |
|---|---|---|
| Hot reducing HCl / H₃PO₄ | good | best |
| Wet chlorine, hypochlorite, ClO₂ | best | good |
| Ferric chloride (FeCl₃) | best | good |
| Nitric acid and mixed acids | best | good |
| Chloride pitting and crevice attack | best | good |
| Seawater and marine chlorides | best | good |
| FGD absorber and ducting | best | good |
| Pulp and paper bleach plant | best | good |
The first row is the only one that keeps C-276 in the frame, every oxidising row tilts to C-22. A plant that runs both a bleach line and a hot-acid line is therefore specifying two grades, not one.
PREN ranks C-276 higher, and C-22 still wins in oxidising service
The standard first-approximation index for pitting resistance is PREN = Cr + 3.3 × (Mo + 0.5 W). Taken at the lower bound of each ASTM window, the arithmetic gives:
| Grade | Cr | Mo | W | PREN (lower bound) |
|---|---|---|---|---|
| C-276 | 14.5 | 15.0 | 3.0 | 68.9 |
| C-22 | 20.0 | 12.5 | 2.5 | 65.4 |
By that index C-276 edges ahead, it carries more molybdenum, and the formula weights molybdenum heavily. The apparent contradiction resolves on one point: PREN is a reducing-environment index, and an FGD absorber is not reducing. Scrubber liquor is oxidising (oxidation air, ferric ions from the flue gas), and under an oxidising load the higher-chromium grade holds the passive film while the lower-chromium grade can break down locally. That is why the field answer and the index disagree, and why the correct sequence is: use PREN as a first filter, then let the oxidation state of the actual liquor make the final call.
Envelope, forms and standards
The two grades differ on more than chemistry, the verified service envelope and the standards list diverge too:
| Property | C-22 | C-276 |
|---|---|---|
| UNS | N06022 | N10276 |
| Density | 8.69 g/cm³ | 8.89 g/cm³ |
| Verified service ceiling | 600 °C | 400 °C |
| Governing standards | ASME Section VIII · ASTM B574 · ASTM B575 · NACE MR0175 | ASTM B575 · ASTM B574 · ASTM B564 · UNS N10276 |
| Stock forms | Forging, Wire, Flange, Bar & Rod, Plate & Sheet, Pipe & Tube | Forging, Wire, Plate, Sheet, Strip, Bar, Tube |
The ceiling difference is the underrated line: C-22’s verified envelope reaches 600 °C against C-276’s 400 °C, so where a duty is both corrosive and warm, a preheater, a hot scrubber liquor line, a bleached-stock contact, C-22 carries the higher temperature qualification on top of the oxidising advantage. On the pressure side, C-22’s ASME Section VIII listing is the same code basis a vessel fabricator already designs to.
Specify it, then verify it
Both grades weld readily, with the matching filler: ERNiCrMo-10 for C-22 and ERNiCrMo-4 for C-276. C-276’s documented advantage is that it needs no post-weld heat treatment. C-22 extends the same low-carbon, weld-clean design to oxidising duty. Write the order as: grade + UNS, the form and its standard (ASTM B575 plate, B574 bar, B622 seamless tube, B564 forging), the condition (solution annealed) and the certificate (EN 10204 3.1 heat chemistry, escalating to 3.2 where the project witnesses it), add NACE MR0175 / ISO 15156 wherever the component sees sour service. At goods-in, the verification step that keeps the two apart is OES or spark analysis reported against the B575 window on chromium and molybdenum, reconciled to the marked heat number. Handheld XRF cannot do it, because the discriminator is a ratio, not an element.
How to select the right option for your process
Five checks, in order. Each one keeps the component inside its specification:
- Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
- Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
- Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
- Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
- Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.
Frequently Asked Questions (FAQ)
Is Hastelloy C-22 a direct replacement for C-276?
In oxidising and mixed-acid service, usually yes, C-22 is the standard upgrade for FGD, bleach plants and pharmaceutical vessels. In strongly reducing hot hydrochloric acid, keep C-276: its higher molybdenum is the property that duty needs. Decide on the oxidation state of the liquor, not on the grade name.
Which is more corrosion resistant, C-22 or C-276?
Neither is universally more resistant. C-22 (20.0-22.5 % Cr) wins in oxidising chloride media, wet chlorine, hypochlorite, ferric chloride, FGD liquor. C-276 (15.0-17.0 % Mo) wins in strongly reducing hot acids. The pitting index PREN favours C-276 (68.9 against 65.4 at the lower bound of each window), but PREN assumes reducing conditions, which is precisely the assumption an oxidising scrubber breaks.
Can a handheld XRF tell C-22 from C-276?
No. Both are Ni-Cr-Mo alloys that also contain tungsten, so no single element separates them. The discriminator is the chromium-to-molybdenum ratio, C-276 at 14.5-16.5 % Cr with 15.0-17.0 % Mo against C-22 at 20.0-22.5 % Cr with 12.5-14.5 % Mo, which needs OES or spark analysis reported against the ASTM B575 window and reconciled to the heat number.
Which grade runs hotter?
C-22: its verified service ceiling is 600 °C against C-276’s 400 °C. Where a corrosive duty is also warm, that higher temperature qualification is a second reason C-22 is specified, and above C-276’s ceiling its datasheet guarantee ends regardless of how good the corrosion resistance is.