GH3044 vs Inconel 625 vs Hastelloy X
Three nickel-chromium alloys that get quoted against each other constantly. They are not interchangeable, and the difference is written in the tungsten, molybdenum and niobium lines.
The 30-second answer
§01, SummaryGH3044
Cheapest to 900 °C
14.5–16% tungsten does the strengthening. No molybdenum, no cobalt. The domestic combustion-chamber grade under GB/T 14992.
Hastelloy X
Hottest at 1100 °C
Cobalt plus 17–20% iron plus molybdenum. Furnace and gas-turbine duty where creep and oxidation at temperature decide the part.
Inconel 625
Only one for chlorides
Molybdenum plus niobium buys pitting and crevice resistance, and it welds without PWHT. 980 °C ceiling, NACE MR0175 listed.
Side by side, to the specification
§02, ChemistryEvery line below is the specification range, not a nominal figure from a datasheet. GH3044 is quoted to GB/T 14992, Hastelloy X to ASTM B435/B572 and AMS 5536, Inconel 625 to ASTM B443/B444/B446.
| Specification item | GH3044 | Hastelloy X | Inconel 625 |
|---|---|---|---|
| UNS | N06604 | N06002 | N06625 |
| Governing spec | GB/T 14992 | ASTM B435 / B572 · AMS 5536 | ASTM B443 / B444 / B446 |
| Nickel | Balance | Balance | 58.0 min |
| Chromium | 23.5–26.5 | 20.5–23.0 | 20.0–23.0 |
| Molybdenum | — | 8.0–10.0 | 8.0–10.0 |
| Tungsten | 14.5–16.0 | 0.2–1.0 | — |
| Iron | 4.0 max | 17.0–20.0 | 5.0 max |
| Cobalt | — | 0.5–2.5 | — |
| Niobium + Ta | — | — | 3.15–4.15 |
| Carbon | 0.10 max | 0.05–0.15 | 0.10 max |
| Density | 8.89 g/cm³ | 8.22 g/cm³ | 8.44 g/cm³ |
| Melting range | ≈1380–1410 °C | 1325–1360 °C | 1290–1350 °C |
| Max service temp | 900 °C | 1100 °C | 980 °C |
| Cost vs 316L | 2–3× | 4–6× | 3–4× |
Units in wt %. “Balance” means the remainder after the specified elements. The widest single divergence in the table is tungsten: 14.5–16.0% in GH3044 against 0.2–1.0% in Hastelloy X — that one line explains most of the behavioural difference between them.
What each element is actually doing
§03, MechanismTungsten — strength without ageing
A heavy, slow-diffusing atom that stiffens the nickel matrix. It lets GH3044 hold creep strength at 900 °C while staying single-phase, so it welds and is never heat-treated after fabrication. What it does not do is resist aqueous chlorides.
Molybdenum — corrosion, and some strength
The element that raises resistance to pitting and crevice attack. In Hastelloy X it works alongside cobalt for high-temperature duty; in Inconel 625 it is the corrosion workhorse. Its price moves on its own market, which is why both alloys re-price when molybdenum does.
Niobium — the 625 discriminator
3.15–4.15% Nb+Ta in 625 stiffens the matrix alongside molybdenum and delays the onset of the strengthening you would otherwise need ageing to get. Neither GH3044 nor Hastelloy X specifies it, which is why neither is the grade for sour or chloride duty.
Five enquiries, five answers
§04, ScenariosFurnace internals, 950–1100 °C, oxidising, cyclic
→ Hastelloy XCobalt plus the wider chromium-to-iron balance gives it the best creep and oxidation combination in this group at 1100 °C. GH3044 tops out near 900 °C and 625 near 980 °C — above those the oxide scale starts to spall on thermal cycling.
Aero engine combustion chamber, domestic programme, 850–900 °C
→ GH304414.5–16% tungsten is the cheapest way to get solid-solution strength at temperature inside a Chinese supply chain, and GB/T 14992 is what the drawing will call out. It is the standard combustion-chamber sheet grade in domestic engine work.
Seawater flange, chemical vessel, or weld repair in the field
→ Inconel 625Neither GH3044 nor Hastelloy X is the right answer here. Molybdenum plus niobium is what buys pitting and crevice resistance in chlorides, and 625 welds without post-weld heat treatment — which matters when you cannot re-heat-treat an installed part.
Sour gas line, NACE MR0175, 120 °C
→ Inconel 625625 is listed for sour service under NACE MR0175 subject to hardness limits. GH3044 and Hastelloy X are not the grades your certification body will expect for this duty.
Cost reduction review on an existing Hastelloy X part at 880 °C
→ Test GH3044Below roughly 900 °C the tungsten-bearing GH3044 covers the same duty at a lower metal cost, because it strips out the cobalt and most of the iron-molybdenum stack. Qualify it on a creep test at your actual temperature before switching production, not on data sheet maxima.
Why the price ordering is not obvious
§05, CostGH3044 is usually the cheapest of the three and Hastelloy X the most expensive, but the gap is narrower than buyers expect, and it is not stable — it moves with nickel, molybdenum and cobalt separately.
GH3044 carries no molybdenum and no cobalt
That removes the two most volatile cost lines after nickel itself, so its price is comparatively stable — which is a real advantage when you are budgeting a furnace rebuild six months out.
Hastelloy X carries cobalt
Cobalt is a separate, thin, battery-driven market. When it moves, Hastelloy X moves with it for reasons that have nothing to do with your furnace, which is why quotes on this grade need a shorter validity window.
For per-kilogram reference bands on 625 specifically, see the Inconel 625 price guide. The same cost build-up logic applies to the other two, with the element lines swapped.
How to write the purchase order
§06, ProcurementGrade plus standard, always. "Hastelloy X, ASTM B435" is a purchase order. "Hastelloy X sheet" is an invitation to a dispute.
State the service temperature. It is the single fact that decides whether GH3044 can replace Hastelloy X on your part.
State the atmosphere. Oxidising, reducing, carburising and chloride-bearing duties point at different grades even at the same temperature.
Name the condition. Annealed, solution treated and cold worked sheet are not interchangeable, and the certificate must match.
Eight questions buyers ask
§07, QuestionsIs GH3044 the same as Hastelloy X?
No, but they are cousins. Both are nickel-chromium alloys for high-temperature oxidation duty and both rely on solid-solution strengthening rather than ageing. GH3044 reaches its strength with 14.5–16% tungsten under GB/T 14992; Hastelloy X uses 8–10% molybdenum, 17–20% iron and 0.5–2.5% cobalt under ASTM B435/B572. Substituting one for the other requires a creep test at your service temperature, not a chemistry comparison.
Which of the three is best for 1000 °C?
Hastelloy X. Its 1100 °C rating is the highest of the group. Inconel 625 is rated to 980 °C and GH3044 to about 900 °C. Above 980 °C, 625 loses the advantage that justifies its price, because the corrosion resistance it is bought for is not the limiting property at that temperature.
Can I use Inconel 625 instead of Hastelloy X to save cost?
Only if your service temperature sits comfortably below 980 °C and the duty is corrosion-led rather than creep-led. The two alloys cost in a similar band, so there is rarely a large saving; the real difference is which property you are paying for. If the part is a furnace support at 1050 °C, 625 is the wrong purchase regardless of price.
Why does GH3044 contain so much tungsten?
Tungsten is a heavy, slow-diffusing atom. Dissolved in the nickel matrix it raises creep resistance at temperature without needing an ageing treatment, which keeps the alloy weldable and single-phase. 14.5–16% is high enough to do real work, which is why GH3044 holds strength to 900 °C despite having no molybdenum at all.
Do all three weld without post-weld heat treatment?
They are all weldable, and none of them is age-hardened, so none demands a post-weld ageing cycle. Inconel 625 is the one most often chosen precisely because it can be welded in place on installed equipment. For Hastelloy X and GH3044 in thick sections, a solution anneal after welding is still worth discussing with the fabricator.
Which grade resists chlorides best?
Inconel 625, by a clear margin, because of the molybdenum-niobium combination. Hastelloy X contains molybdenum but is formulated for oxidation and creep at temperature rather than for aqueous chloride service, and GH3044 has no molybdenum at all. If the duty involves seawater or wet chlorides, the comparison stops being about temperature.
Can you supply all three from one order?
Yes. GH3044, Hastelloy X and Inconel 625 are all within the 37 grades we hold routes for, in sheet, plate, bar, forging and wire. What differs is the certificate basis: GB/T 14992 for GH3044, ASTM B435/B572 or AMS 5536 for Hastelloy X, ASTM B443/B444/B446 for 625.
How do I write the purchase specification so I get the right one?
State the grade and the standard together — for example 'Hastelloy X, ASTM B435, annealed, 3 mm sheet' — plus the service temperature and atmosphere. A purchase order that says only 'Hastelloy X sheet' leaves the mill free to choose the condition, and the condition is often what determines whether the part survives thermal cycling.
Not sure which of the three fits?
Send the part, the service temperature and the atmosphere. If a cheaper grade does the job we will say so — the quote will name the grade we recommend and the standard it is made to.
Describe the duty — get a grade recommendation